Calco Poly Technik

Home / Materials / Processing guidelines

Typical starting conditions for injection moulding.

Starting points for standard reinforced grades, family by family, with the practice notes that prevent most moulding problems.

By family.

FamilyDryingMax. moistureMelt temperatureMould temperature
CiLON® / eCiLON® PA680 °C, 4–6 h≤ 0.10%240–270 °C60–90 °C
CiLON® / eCiLON® PA6680 °C, 4–6 h≤ 0.10%275–295 °C70–100 °C
ZiLITE® PBT and alloys120 °C, 3–4 h≤ 0.04%240–260 °C60–100 °C
NovaLYN™ mPPE100 °C, 2–4 h≤ 0.05%280–310 °C80–110 °C
HiLENE® PPNot normally required—200–240 °C20–60 °C
PiCAN® PC120 °C, 3–4 h≤ 0.02%280–310 °C80–110 °C
PiCAN® PC/ABS100 °C, 3–4 h≤ 0.04%240–270 °C60–80 °C

Starting points for standard reinforced grades. The grade data sheet and, where issued, the product-specific processing sheet take precedence: flame-retardant, high-flow and alloy grades run in narrower windows.

Practice notes.

Dry properly, then keep it dry

Use dehumidified-air or vacuum hopper dryers and measure air temperature at the hopper inlet. Material above the moisture limit will degrade in the barrel: splay, brittleness and out-of-tolerance parts follow.

Watch residence time

Long hold-up at maximum melt temperature degrades every thermoplastic and, for flame-retardant grades, can release irritant vapours. Size the shot to the machine and purge with PE or PS on every stop.

Mould temperature is a property

Crystallinity, surface finish, shrinkage and post-moulding dimensional stability all follow mould temperature. Insulate the tool and keep the inlet-to-outlet coolant difference under 5 °C.

Vent, draft and gate

Vent cavities and runners at the parting line (land of 0.8 mm or less); draft 0.5–1° per side; gate so weld lines fall away from load-bearing bosses in glass-reinforced grades.

Regrind with care

Clean, dry, sorted regrind can be blended back in most grades; determine the permissible proportion by trial, as impact strength, flow and surface finish can shift with small additions.

Safety

Melts can cause severe burns and, if overheated, gas pressure behind the nozzle. Use purge shields and gloves, provide local exhaust at the barrel, and clean spilled pellets immediately.

A problem at the press?

Our application engineers support mould trials on site.